Umumy maksatly fluoroelastomer esasly polimer
Stok nusgasy mugt we elýeterlidir
“Viton FKM” çig sagyz witon kauçugynyň çig mallarydyr. Biz Hytaýda “Low Mooney”, “Middle Mooney” we “High Mooney” görnüşlerini öz içine alýan iň ýokary hilli “Viton FKM” çig sagyzlaryny üpjün edýäris.
FD26 seriýaly FKM çig sakgyjy winiliden ftoridden (VDF) we geksaftorpropilenden (HFP) düzülen bir görnüşli kopolimerdir. Bu umumy netijeliligi gowy görkezýän standart FKM görnüşidir. Materialyň umumy häsiýetlerini aşakdaky tablisadan tapyp bilersiňiz.
| Äzajylar | Bahalar | ||||
| FD2601 | FD2602 | FD2603 | FD2604 | FD2605 | |
| Dykyzlyk (g/sm3)3) | 1.82±0.02 | 1.82±0.02 | 1.82±0.02 | 1.82±0.02 | 1.82±0.02 |
| Ftoryň mukdary (%) | 66 | 66 | 66 | 66 | 66 |
| Muni ýapyşyklygy (ML (1+10)121℃) | 25 | 40~45 | 60~70 | >100 | 150 |
| Gurlandan soň dartgynlylyk güýji (Mpa) 24 sagat, 230℃ | ≥11 | ≥11 | ≥11 | ≥13 | ≥13 |
| Gurlandan soň arakesmede uzalma (%) 24 sagat, 230℃ | ≥180 | ≥150 | ≥150 | ≥150 | ≥150 |
| Kompressiýa toplumy (%) 70 sagat, 200℃ | ≤25 | ||||
FD24 seriýaly FKM çig sagyz winiliden ftoridinden (VDF), geksaftorpropilenden (HFP) we tetraftoretilenden (TFE) ybarat bolan bir görnüşli terpolimerdir. Terpolimerler kopolimerlere garanyňda (adatça 68 we 69 agram prosent ftor aralygynda) has ýokary ftor mukdaryna eýedir, bu bolsa
himiki we ýylylyk garşylygyny ýokarlandyrýar. Materialyň umumy häsiýetlerini aşakdaky tablisadan tapyp bilersiňiz.
| FD2462 | FD2463 | FD2465 | FD2465L | FD2465H | |
| Ftoryň mukdary | 68.5 | 68.5 | 68.5 | 65 | 69.5 |
| Dykyzlyk (g/sm3)3) | 1.85 | 1.85 | 1.85 | 1.81 | 1.88 |
| Muni ýapyşyklygy (ML (1+10)121℃) | 70±10 | 40±10 | 45±15 | 50±10 | 40±20 |
| Gurlandan soň dartgynlylyk güýji (Mpa) 24 sagat, 230℃ | ≥11 | ≥11 | ≥11 | ≥11 | ≥11 |
| Gurlandan soň arakesmede uzalma (%) 24 sagat, 230℃ | ≥180 | ≥180 | ≥180 | ≥180 | ≥180 |
| Kompressiýa toplumy (%) 200℃ 70H kompres 20% | ≤30% | ≤30% | ≤30% | ≤30% | ≤40% |
| Ýaga garşylyk (200℃ 24H) RP-3 ýagy | ≤5% | ≤5% | ≤5% | ≤5% | ≤2% |
| Aýna geçiş temperaturasy (TG) | >-15℃ | >-15℃ | >-15℃ | >-21℃ | >-13℃ |
| Suwuň mukdary (%) | ≤0.15 | ≤0.15 | ≤0.15 | ≤0.15 | ≤0.15 |
Paket we Saklama
Fluoroelastomerler ilki her bir halta 5 kg agramly PE haltalara gaplanýar, soňra karton gutusyna salynýar. Gutynyň arassa agramy: 25 kg
Fluoreolastomer sowuk, gurak we howa çalynýan ýerde saklanmaly. Ýaramlylyk möhleti öndürilen senesinden başlap 24 aý.